Home / Public case studies / Pipeline seam weld, San Bruno
Industrial · Public case studyPipeline seam weld, San Bruno
NTSB/PAR-11/01 · September 9, 2010 · San Bruno pipeline rupture: the pup 1 seam weld
A step-by-step look at the laboratory evidence behind the rupture of PG&E’s Line 132 in San Bruno, California, on September 9, 2010, as the National Transportation Safety Board (NTSB) examined it: six short pipe pieces, one partially welded seam, and where the fracture began.
Interactive 3D · PDF annex (2.8 MB) · Video (1 min 50)
Key details from the source record
- Presentation
- Independent illustration of public NTSB findings (NTSB/PAR-11/01). Schematic geometry, the 20× enlarged weld sections and representative pup lengths are identified as such.
- Report
- NTSB Pipeline Accident Report NTSB/PAR-11/01, adopted August 30, 2011; investigation DCA10MP008
- Accident
- About 6:11 p.m. Pacific daylight time, a 30-inch natural gas transmission pipeline, Line 132, ruptured at mile point 39.28 in a residential area of San Bruno (p. x)
- Consequences
- "Eight people were killed, many were injured, and many more were evacuated from the area." The fire destroyed 38 homes and damaged 70 (p. x)
- The pipe
- Installed in 1956; recorded by PG&E as seamless X42 pipe, records "which were later found to be incorrect" (p. 1)
Step-by-step reconstruction sequence
The NTSB laboratory evidence step by step, from six short pipe pieces to one partially welded seam
- Step 01
Six pups between two long joints
The NTSB examined the ruptured center section and the cutouts south and north of it. Between two long joints sat six short pipe pieces, "pups", numbered 1–6 from south to north and joined by girth welds C1 to C7 (p. 39).
Pups 1–5 are drawn 45 in each, a representative length inside the reported range, so the positions of C2–C7 are approximate. One quarter of each pup is cut away to show the wall: an inspection view, not damage. The long joints are not drawn, and these six pups are not the 27 ft 8 in center section of Fig. 18.
- Step 02
Three kinds of seam in six pups
The longitudinal seams differed. Pups 1–3 were welded along the outer portion only, leaving an unwelded inner region along the entire seam; pups 4 and 5 had an outer fusion weld and a manual inner weld; pup 6, like the long joints, was standard factory-made DSAW pipe (pp. 41, 43).
The gold rails mark the seams for reading; they are annotations, not weld caps, and are all drawn on top of the pipe. Pups 1, 2, 3 and 5 were rolled in the transverse (nonstandard) direction; pup 4’s chemistry was "consistent with steel made from recycled scrap material" (p. 46).
- Step 03
Pup 1: welded from the outside only (20×)
Cut across, the pup 1 seam shows weld metal only along the outer portion and an unwelded region beneath it. Grinding had removed the weld reinforcement and part of the pipe body, leaving a net intact seam of 0.162 inch (p. 41).
Only the intact seam thickness and the 15° misalignment are fixed from the report; the weld outline, the ground surface and the width of the unwelded gap are schematic. "The unwelded region defect was observed during a visual weld inspection of each pup." (p. 41)
- Step 04
A 15° misalignment, and a notch at the root (20×)
Across the pup 1 seam, the inner surfaces met at a 15° angle (p. 41). The NTSB found that the unwelded portion "formed a notch, the shape of which further concentrated the stresses at the root of the weld", and that the misalignment "added additional bending stresses and strains" (p. 92).
The 15° is drawn as 7.5° on each side of the seam: the split is illustrative, the total is the report’s. The dashed line continues one inner surface across the seam. No stress field is drawn.
- Step 05
Where the rupture began
The fracture features were "consistent with the rupture initiating at a preexisting 2.4-inch-long crack in the pup 1 longitudinal seam 20.3–22.7 inches north of the C1 girth weld (approximately mid-span)" (p. 43).
The red marker’s length and its position along the pipe are the report’s; its width and its place around the circumference are illustrative. The rupture opened the east side of the pipe (p. 93).
- Step 06
Two kinds of growth before the rupture (20×)
Under the microscope, the crack had grown in two ways before the rupture: first by ductile fracture from the root of the weld (stage 1), then by fatigue (stage 2). The rest of the seam broke in the rupture itself, mostly by quasi-cleavage fracture (stage 3) (p. 43).
The opening is an illustrative reveal of the seam face, not the fracture path. The report gives no crack depths, growth rate or cycle count.
- Step 07
386 psig was enough
At the rupture site the pressure was 386–386.4 psig, below the 400 psig maximum allowable operating pressure (p. 91). A properly built 30-inch X42 pipe had an estimated burst pressure of 1,300 psig; the weld defects "reduced the weld strength for pups 1, 2, and 3 by as much as 66 percent" (p. 92).
These are the NTSB’s estimates, made before the crack growth. They cannot account for the misalignment; the pup 1 burst pressure "was likely less than the pup 3 burst pressure" (p. 92). Nothing on this page is computed.
- Step 08
When the crack began: undetermined
"The NTSB investigation was unable to determine when or how the preexisting crack along the intact portion of the pup 1 longitudinal seam initiated." The 386 psig of the rupture day was the highest confirmed pressure there (p. 93).
The three possibilities are the report’s list (p. 94). The page shows no date, no cause and no growth history for the crack.
- Step 09
For comparison: a full-penetration DSAW seam (20×)
Pup 6 and both long joints were standard factory-made DSAW pipe, welded outside and inside: "The outer and inner weld passes overlapped, resulting in full penetration in the joint" (p. 41). No cracks or surface-connected defects were found on these seams.
A typical comparison section, not pup 6 itself, not a repair proposal and not a demonstration of load capacity. The straight boundary between the passes simplifies passes that overlapped and fused.
- Step 10
Same wall, two seams (20×)
At the same 20× enlargement: in pup 1, 0.162 inch of weld held the seam over an unwelded region; in a typical DSAW seam, two overlapping passes fused the full 0.375-inch wall (pp. 41-42).
Both sections are schematic: their proportions are fixed only where the report gives a number. Values are actual sizes.
- Step 11
What the NTSB found
The NTSB concluded that the fracture "originated in the partially welded longitudinal seam of pup 1, which was progressively weakened due to ductile crack growth and fatigue crack growth" (finding 5, p. 124).
Findings quoted in full (p. 124); the probable cause quoted in part, with contributing factors on pressure testing, oversight, valves and emergency response (p. 127). Corrosion was not a factor (finding 1).
- Step 12
Sources and method
One source: NTSB/PAR-11/01, adopted August 30, 2011 (ntsb.gov, investigation DCA10MP008). The pipe and the two weld sections are schematic models built from the report’s dimensions; every page cites its pages and figures.
Independent illustration of public NTSB findings (NTSB/PAR-11/01). Schematic geometry, the 20× enlarged weld sections and representative pup lengths are identified as such. No affiliation with or endorsement by the NTSB or PG&E. Not a new engineering analysis and no opinion on admissibility.
Source & limitations: Shapes, positions and dimensions in the reconstruction are indicative; the report prevails.
From the laboratory examination (pp. 39-46) and the analysis (pp. 92-95). Not affiliated with or endorsed by the NTSB or PG&E.